Two challenges with FDM 3D Printers are:
1. Getting the object to stick to the build plate during printing; failure can result in warping or even complete print failure
2. Removing the object once it's finished
I read all sorts of differing advice on the internet. After some experimentation, I found that it's actually easier than a lot of the advise I was reading (at least for PLA and PET plastics).
In brief:
1. Raise the build plate temperature. About 10⁰C (18⁰F) above recommended values worked for me, although larger parts needed a brim (a thin outline drawn around the bottom). Here are my settings (in Simplify 3D):
- 1st layer height 90% (squishes down the first layer to make it stick)
- Build plate temperature: 70⁰C (158⁰F) for PLA & 80⁰C (176⁰F) for PET
2. Simply wait for the build plate to cool down to below about 30⁰C (86⁰F), and the part easily comes off the build plate (assuming there' a place you can grab hold of it securely)
NOTE: You'll have to experiment with your printer, because different printers have different characteristics and calibrations (e.g., the temperature sensors may not be calibrated properly). Also, I've only tested this with PLA & PET. It might not work with other plastic types.
More articles, videos, etc.:
https://keasigmadelta.com/blog/...